Max Kopp Tech

Building a GeSe Photodetector on PET, Step by Step

Contact Max Kopp
Share Post :

Building a GeSe Photodetector on PET, Step by Step

The flexible GeSe photodetectors in my 2024 paper start with a crystal, a roll of tape, a small block of PDMS and a PET film that already carries gold electrodes. Everything in the device follows from one design decision: put the electrodes down first, then place the semiconductor on top of them, so that nothing harsh ever touches the plastic afterwards. In the paper the finished detectors responded to polarized light with a sinusoidal photocurrent, and I used them to read glucose in solution. This post goes through how they are built, and I have tried to say for each step why it is done that way and what I would still like to measure.

Three steps, three photographs

The paper describes the process in three moves. The photograph below shows each of them.

Three panels: a PET film with gold cross-finger electrodes held in a gloved hand, an exfoliated GeSe crystal on tape, and a microscope image of the GeSe crystal transferred onto the electrodes.
(a) PET substrate with pre-defined cross-finger electrodes. (b) GeSe crystal exfoliated with Nitto tape. (c) Microscope image of the crystal transferred onto the electrodes. Figure from Kopp, M. B., Applied and Computational Engineering 72 (2024) 45–58, doi.org/10.54254/2755-2721/72/20240981, CC BY 4.0.

The first step is the substrate. It is a PET film on which cross-finger gold electrodes have been defined in advance, with a spacing of 60 μm between neighbouring fingers. Panel (a) shows it curved over a gloved hand. The second is the semiconductor. GeSe flakes are mechanically exfoliated with Nitto tape from single crystals supplied by HQ Graphene. Panel (b) shows an exfoliated crystal on the tape. The third is the transfer. A flake is moved from the tape onto the PET with a PDMS-assisted dry transfer, so that it lies across two adjacent electrode fingers. Panel (c) is a microscope view of one in place. Once a flake bridges two electrodes, the device is a metal–semiconductor–metal photodetector, and the bridge is the entire active region.

After the transfer the device is heated at 60 °C for 5 minutes on a hotplate to improve the contact between metal and semiconductor.

Why exfoliate and why a dry transfer

Mechanical exfoliation works on layered materials because the layers are held to each other by weak van der Waals forces, so tape can peel them apart and leave flakes with clean, flat faces. The method gives few flakes and wide variation in thickness and size. Against that, it needs no growth furnace, no high-temperature substrate, and no solvent. For a research device that has to land on plastic, that is the deciding advantage.

The transfer step exists for the same reason. PET cannot go through the baking, etching and wet chemistry that a lithographically patterned device on silicon would see. A dry transfer lets the flake travel from a place where it was made to a place where it could not have been made. As I understand the general technique, a flake is picked up from the tape onto a soft PDMS stamp, inspected under a microscope, aligned over the target and pressed down, and the stamp is lifted away while the flake stays on the surface. The adhesive on the tape is a contaminant I do not want at the electrical contact, and PDMS generally leaves less residue there. I have not quantified residue, so I give no number for it.

Why 60 μm and why 60 °C

Both numbers are trade-offs, and both come with a calculation.

In a photoconductor of channel length L under bias V, the photocurrent can be written as I = e η (P / hν) (μ τ E / L), where η is the quantum efficiency, P the optical power, μ the carrier mobility, τ the carrier lifetime and E the field in the channel. That is equation (6) in the paper. The factor μτE/L is the photoconductive gain, which is the carrier lifetime divided by the time a carrier needs to cross the gap. Substituting E = V/L, the gain goes as μτV/L². The gain therefore rises with the square of how much you shrink the gap. As an illustration, a 10 μm gap with everything else equal would give 36 times the gain of a 60 μm gap, since (60/10)² = 36.

If shorter gaps are better, why did I use 60 μm? Because the flake has to bridge the gap. Exfoliated flakes come in whatever size they come in, and a gap that is too wide means few flakes will reach across it, while a gap that is too narrow means careful placement and a higher chance of shorting the device. The geometric argument says to go as small as the flakes and my hands would allow. The practical answer was 60 μm. For an illustrative 1 V bias that gives a field of about 1.7 × 10⁴ V/m, or 167 V/cm.

The 60 °C choice is bounded from above by the plastic. PET softens in the region of 70 to 80 °C, so a hotter anneal could warp the substrate, and 5 minutes at 60 °C is a safe treatment that still improves the contact. A metal–semiconductor contact with a barrier gives a current–voltage curve that bends upward instead of lying on a straight line, and a better contact straightens it. One open question is how far the anneal can be pushed, at what temperature and for how long, before the substrate and not the contact sets the limit.

How I characterized a device

Each detector was measured in an optical darkroom at room temperature. A red laser passed through a polarizer and a half-wave plate that together set the polarization, and a Keithley 2450 source meter measured the current. Current–voltage curves were recorded in the dark and under a 5 mW laser. To get the polarization response, the half-wave plate was rotated from 0° to 180° and the photocurrent was recorded at each step, giving a curve that I fitted with a sinusoid of the form I₀ + I_A sin(2θ + φ). For glucose, the sample was placed in the beam path between the plate and the detector, and the same scan was repeated. The same scan has a second use that I find easy to overlook. Unless the flake’s axes are known before it is placed, the angle at which the photocurrent peaks also tells me where the crystal’s armchair axis lies for that device.

A quick check on the photon budget

At an illustrative red wavelength of 650 nm, a photon carries 1240/650 ≈ 1.9 eV, or 3.1 × 10⁻¹⁹ J. A 5 mW beam therefore delivers about 1.6 × 10¹⁶ photons per second. If every photon produced exactly one electron in the external circuit, the current would be e times that, about 2.6 mA. A photoconductor on a single flake delivers far less than that, and most of the difference is geometric.

Here is an illustration with assumed sizes, since I am not quoting a beam diameter. A beam 1 mm across has an area of about 8 × 10⁻⁷ m². A flake 50 μm across has an area of about 2.5 × 10⁻⁹ m². If the beam is not focused, only about 0.3% of the light lands on the flake. The rest of the difference comes from a flake that is thin and absorbs only a fraction of what hits it, carriers that recombine before the contacts collect them, and a gain below its geometric maximum. Separating those factors takes a measurement I would like to make: focus the beam onto the flake and record the photocurrent against the power that actually reaches it. That gives a responsivity per unit of absorbed light, which is the number that lets one flake be compared with another.

What flexible means here

Left: a finished GeSe sensor on a flexible film. Right: the film held between two fingertips and bent.
Photograph of the fabricated GeSe-based sensor. The device can be freely bent. Figure from Kopp, M. B., Applied and Computational Engineering 72 (2024) 45–58, doi.org/10.54254/2755-2721/72/20240981, CC BY 4.0.

The photograph shows that the device can be bent freely, which is a statement about handling. Quantifying it is the next step: a bending radius, a number of cycles, and the change in photocurrent after bending. A layered crystal bonded by van der Waals forces on a film that bends elastically is a good starting point for that test, and whether the contact survives thousands of flexes is the question the test would answer.

Next measurements: device-to-device statistics

The paper demonstrates devices that work. The step beyond a working device is describing the spread between devices, and I would do that with a per-device table: flake thickness from atomic force microscopy, the orientation found from the polarization scan, the dark current at 1 V, and the photocurrent at a fixed absorbed power. Add the fraction of transfers that produced a usable device. Five or ten devices in a table would say more about the method than any single good curve, and it is the data a group trying to repeat the fabrication would need first.

Sources and links