The ultrasonic sensors in my structural-monitoring project are made on an ordinary desktop inkjet printer, an Epson R230, with silver nanoparticle ink laid down as electrodes on polymer films. For the piezoelectric version the film is PVDF, and the electrodes go on both faces. I also built triboelectric versions from stacked polymer layers. This post is about the engineering reasoning behind a printed sensor, and I have mostly kept it to arithmetic that anyone can redo. The full study is in a manuscript that has not yet been published in a journal, so here I stay with methods, simple models and the literature, and leave measured results to the paper.

Why print a sensor at all

A catalogue ultrasonic transducer is a good device and a poor match for what I wanted. It is bulky, it senses at a single point, and it is rigid, so it does not follow a curved wall. The aim of the project is an array of sensors laid onto a surface where a defect is likely, such as a joint or a weld, and made when it is needed. An inkjet deposits a pattern wherever the file says, on a flat sheet today and, in principle, onto something curved later. That makes it a natural way to produce an array whose layout can change.

The printer and the ink

The first decision was how much printer to use. I wanted to find out whether a household printer would do, and I chose the Epson R230. Its print head is itself piezoelectric, with a piezo element squeezing each nozzle, so the ink is dosed drop by drop under electrical control. That is a pleasing symmetry, and it also matters: a piezo head ejects the ink without heating it, which is gentler on both the ink and a heat-sensitive film.

A desktop inkjet printer with three small printed sensor pieces on top and a long printed sheet with dark stripes emerging from the front.
Printed pieces and a printed sheet at the printer. Photograph by the author, also shown on maxkopptech.com/space-monitoring/.

The ink was the second decision. A silver precursor ink can form highly conductive patterns through electroless plating, but it needs a post-anneal and can suffer from uniformity problems. A silver nanoparticle ink is more stable and can be formulated to the viscosity and surface tension that a household printer is built for. I used a silver nanoparticle ink from Mitsubishi Paper Mills. The constraint that shapes the choice is the film underneath. PVDF’s piezoelectric response comes from a poled crystalline phase, and datasheets typically limit use to somewhere around 80 to 100 °C. An ink that needs a hot sintering step therefore competes with the film’s own temperature limit, and inks that sinter at low temperature on a coated substrate are the natural partner. How much a given process degrades the response is something to measure, not assume.

A printed element is a capacitor

Two metal layers either side of a dielectric film make a capacitor, and a piezoelectric film is a capacitor that also generates charge when strained. That gives a circuit model simple enough to do on paper, with every number below an illustrative assumption.

Take a film 28 μm thick with a relative permittivity of about 12, which are typical datasheet values for PVDF, and an electrode overlap of 10 mm by 10 mm. The capacitance is ε₀ ε_r A / t, about 380 pF. At 50 kHz, an illustrative drive frequency, the reactance of that capacitance is about 8.4 kΩ, so the sensor looks like a high-impedance source.

Circuit diagram: a voltage source in series with the sensor capacitance, feeding the cable capacitance, the scope input capacitance and the scope input resistance in parallel to ground.
Equivalent circuit of a printed piezoelectric element read by an oscilloscope, with illustrative values. Schematic and arithmetic by the author; no measured data.

Connect it to an oscilloscope through a 1 m coaxial cable of about 100 pF, into an input of 1 MΩ and 15 pF. The sensor capacitance and the load now form a capacitive divider, and the voltage at the scope is the open-circuit voltage multiplied by C_s / (C_s + C_c + C_in), which is 0.77. The corner of the resulting high-pass filter is at 1 / (2π R_in (C_s + C_c + C_in)), about 320 Hz, far below an ultrasonic signal. Loading by the cable costs a quarter of the signal, and the 1 MΩ input costs nothing in this band.

The same arithmetic shows a trap. If I shrink the electrode overlap to 5 mm by 5 mm, the capacitance falls fourfold to about 95 pF and the divider falls to 0.45. The open-circuit voltage of a piezoelectric film does not depend on its area, but the voltage a reader sees does, as soon as the cable is comparable to the sensor. A small printed pixel on a long lead wastes more than half its signal unless the first amplifier sits close to it. This is why I think of a printed sensor and its preamplifier as one design.

How much voltage per nanometre?

For a thin film bonded to a surface, the film is much thinner than the wavelength, so it simply follows the strain of the plate. The open-circuit voltage is V = g₃₁ · T · t, where T is the stress along the film’s stretch direction and g₃₁ is the voltage coefficient. A typical datasheet value for PVDF is about 0.22 V·m/N, and its modulus is a few GPa, so take 3 GPa.

Assume an illustrative surface displacement of 1 nm at 50 kHz in a wave travelling at 5 km/s. The wavelength is 100 mm, the strain is 2π/λ times the displacement, about 6 × 10⁻⁸, and the stress is about 190 Pa. The open-circuit voltage is then 0.22 × 190 × 28 × 10⁻⁶, about 1.1 mV, and with the divider above it is about 0.9 mV at the scope. A signal of a nanometre produces a millivolt. Whether that is large or small depends on the source and the noise floor of the reader, and it tells me that sub-nanometre signals need a preamplifier, averaging, or both.

The same picture explains why the aperture of the electrode is not a free choice. A sensor of length L averages the strain over its length, which attenuates the response by sin(kL/2) / (kL/2), where k is the wavenumber. For L = 10 mm and a 100 mm wavelength the factor is 0.98, a loss of under 2%. If the wavelength were 10 mm, the same electrode would average to zero.

Two ways to make a sensor

I built the stacked-polymer triboelectric version as well. Its mechanism is different: two layers touch and separate, charge moves between them, and a voltage appears. It is simple to make, and it raises a mechanical question at ultrasonic frequencies. The surface of the plate accelerates at ω² times its displacement. For 1 nm at 50 kHz that is about 100 m/s², or 10 g. A layer that is only lightly preloaded would be thrown off the surface by motion that small, so a contact–separation sensor at these frequencies depends strongly on preload and coupling. A piezoelectric film converts strain to charge with no moving interface, which makes its response easier to model and, I expect, easier to repeat. I treat that as a hypothesis about the two designs that I would test with a controlled preload, since I have drawn it from the physics rather than from a comparison.

Line width is a printing question

Electrode traces printed from silver ink have a resistance, and it is worth checking whether it matters. Assume an illustrative sheet resistance of 2 Ω per square after sintering. A trace 0.5 mm wide and 50 mm long is 100 squares, so about 200 Ω. Compared with the sensor’s reactance of 8.4 kΩ at 50 kHz, that is 2%. The conductor loss is negligible for a high-impedance source, which means the width of a trace is chosen by how reliably the printer can lay it down, not by electrical needs.

Eight black electrode patterns in two rows, each with two vertical traces ending in square pads and a horizontal line across them, labelled A1 to A4 from 0.1 to 0.4 mm and B1 to B4 from 0.5 to 0.8 mm.
Electrode test patterns labelled by dimension, 0.1 to 0.8 mm, as shown on maxkopptech.com/space-monitoring/. Layout by the author.

That is the reason for test patterns like the ones above, where a feature is repeated at a series of dimensions. Wetting of ink on a low-surface-energy polymer such as PVDF, the drop spacing and the cure all decide the narrowest line that is continuous across a whole film, and the only way to find it is to print a ladder of widths and look.

What I print and what I buy

One distinction sets how far the idea can go. I print the electrodes, and the PVDF film, which carries the piezoelectric property, comes from a supplier. Other groups print the piezoelectric layer too. Thuau and co-workers made all-inkjet-printed piezoelectric devices from P(VDF-TrFE) (2017, doi:10.1039/C7TC02558K). White and co-workers extruded PVDF-trFE films about 40 μm thick, reached a piezoelectric coefficient of up to 25 pC/N, and built an all-printed dynamic force sensor with a sensitivity of 1.18 V/N, explicitly for in-space structural health monitoring (2024, doi:10.1088/1361-665X/ad3d16). Yoo and colleagues used a piezoelectric paint to make two-dimensional phased sensor arrays for thin panels (2010, doi:10.1088/0964-1726/19/7/075017).

Next to those, mine is the most modest on materials and the cheapest on equipment. If the long-term idea is that crew could make sensors on demand, the film becomes the dependency, because someone has to carry it. Printing the active layer as well would remove that, at the cost of the ink, curing and poling work that White and co-workers describe. For now I describe my devices as printed electrodes on a purchased piezoelectric film.

What I would measure next

Voltages from one setup depend on the source, the coupling and the position, so they say little about sensitivity. The first measurement I would add is a calibrated reference transducer in the same place on the same plate, with the printed sensor’s output reported relative to it. The second is the scaling with electrode overlap, which the circuit model above predicts, so a test of it is also a test of the model. The third is adhesion and bending. An electrode that cracks under repeated flexing ends the usefulness of a flexible array. The fourth is temperature, because it acts on the film, the ink, and the wave speed at once. Next experiments for localization itself are in the last post of this series.